European Hydrogen Incidents and Accidents database HIAD 2.1, European Commission, Joint Research Centre
Release from a burst disc (605)
This data is from the European Hydrogen Incidents and Accidents database HIAD 2.1, European Commission, Joint Research Centre.
Release from a burst disc
A burst disc opened prematurely at a research facility, during a hydrogen tube trailer filling operation. The disc failed at 87% (5200 psig, approximately 36 MPa) of the final pressure (6000 psig, approximately 41 MPa). A vent line attached to the burst disc was not sufficiently anchored and bent outward violently from the thrust of the release over an approximate 102 mm (4-inch) moment arm, causing considerable damage to the adjacent vent system components. To continue the operation of filling of the trailer, the damaged portion of the tube bank, consisting of 6 tubes, was isolated by means of valves, and the operation was resumed with the unaffected portion of the tube bank which had another 18 tubes, until a second burst disc failed. The incident investigation revealed that the burs discs were made of pure nickel and affected by extensive hydrogen embrittlement.
The INITIATING CAUSE was the premature failure of a burst disc. The ROOT CAUSE is related to the management shortcoming, allowing the re-installation of a non-hydrogen system for hydrogen purposes, without considering new related risks and the needs for a careful re-assessment of the system for its new uses. DETAILED CAUSE ANALYSIS Metallurgical examination of the two failed burst discs indicated the occurrence of hydrogen embrittlement; they were found to be fabricated from pure nickel with evidence of extensive fracture. An inspection of all vent circuits found that each of the 24 discs in service was made from nickel, were affected by surface fractures which extended around the entire periphery of the rupture disc. Such defects are indicative of hydrogen embrittlement. An inspection of all vent circuits found that each of the 24 discs in service was made from nickel. The storage bank had been employed before for the storage of helium. The pressure vessel documentation accompanying the system indicated that the burst discs were made of stainless steel and rated to 10,000 psig. The damage was caused by the disc vent line which was not well fixed and moved with the hydrogen thrust
We are professional and reliable provider since we offer customers the most powerful and beautiful themes. Besides, we always catch the latest technology and adapt to follow world’s new trends to deliver the best themes to the market.
Contact info
We are the leaders in the building industries and factories. We're word wide. We never give up on the challenges.
The INITIATING CAUSE was the premature failure of a burst disc. The ROOT CAUSE is related to the management shortcoming, allowing the re-installation of a non-hydrogen system for hydrogen purposes, without considering new related risks and the needs for a careful re-assessment of the system for its new uses. DETAILED CAUSE ANALYSIS Metallurgical examination of the two failed burst discs indicated the occurrence of hydrogen embrittlement; they were found to be fabricated from pure nickel with evidence of extensive fracture. An inspection of all vent circuits found that each of the 24 discs in service was made from nickel, were affected by surface fractures which extended around the entire periphery of the rupture disc. Such defects are indicative of hydrogen embrittlement. An inspection of all vent circuits found that each of the 24 discs in service was made from nickel. The storage bank had been employed before for the storage of helium. The pressure vessel documentation accompanying the system indicated that the burst discs were made of stainless steel and rated to 10,000 psig. The damage was caused by the disc vent line which was not well fixed and moved with the hydrogen thrust